Electrospinning: what controls fibre diameter
Electrospinning draws a polymer solution into fibres, typically from about 100 nm to a few µm in diameter, by charging a droplet until electrostatic repulsion overcomes surface tension. A jet leaves the Taylor cone, thins through a whipping instability, dries in flight and is collected as a nonwoven mat.
Start from the solution
For solution electrospinning, solution properties usually set the window in which the instrument settings operate. The most important requirement is sufficient chain entanglement. Below the entanglement concentration the jet breaks into droplets (electrospraying); somewhat above it, beaded fibres form; further above it, smooth fibres become possible. For linear and branched polyesters, McKee and co-workers found that bead-free fibres required concentrations of roughly two to two-and-a-half times the entanglement concentration. Treat that ratio as a starting point for other systems, not a general rule.
Concentration and molecular weight act together. Solution viscosity, measured on a rheometer, is a convenient practical indicator of both, which is why a flow curve of the spinning solution is worth recording before extensive tuning.
Other variables
- Conductivity. More charge carried by the jet generally increases stretching and can reduce fibre diameter; small additions of salt are a common lever. Excessive conductivity can destabilise the jet.
- Solvent volatility. The solvent must largely evaporate in flight. Too slow gives fused or wet fibres; too fast can solidify the polymer at the needle tip. Solvent blends are a common compromise.
- Flow rate. Higher feed rates tend to give thicker fibres and, beyond a limit, beads.
- Voltage. Essential to start and stabilise the jet. Within the stable window its effect on diameter is often smaller than that of the solution variables, and reported trends differ between systems.
- Distance, temperature and humidity. These control drying time and charge dissipation. Humidity is a frequent reason why a previously reliable recipe behaves differently on another day, so record it.
A practical sequence
Treat the problem in two stages: first obtain a solution that spins stably (entanglement, conductivity, volatility, all measurable at the bench), then tune the processing parameters. If a morphology problem persists over a range of voltages, revisit the solution before continuing to adjust the field. A small designed experiment over the solution and processing variables together is often more informative than changing one setting at a time.
References
- S. L. Shenoy, W. D. Bates, H. L. Frisch and G. E. Wnek, “Role of chain entanglements on fiber formation during electrospinning of polymer solutions: good solvent, non-specific polymer–polymer interaction limit”, Polymer 2005, 46, 3372. doi:10.1016/j.polymer.2005.03.011
- M. G. McKee, G. L. Wilkes, R. H. Colby and T. E. Long, “Correlations of solution rheology with electrospun fiber formation of linear and branched polyesters”, Macromolecules 2004, 37, 1760. doi:10.1021/ma035689h
- D. H. Reneker and A. L. Yarin, “Electrospinning jets and polymer nanofibers”, Polymer 2008, 49, 2387. doi:10.1016/j.polymer.2008.02.002