Stress relaxation on CANs: three pitfalls before you fit anything
Covalent adaptable networks are usually characterised by stress-relaxation experiments: apply a step strain, follow the modulus as it decays, extract a characteristic relaxation time τ at several temperatures, fit an Arrhenius law and report an activation energy. Every step of that sequence assumes that the sample is the same material throughout the measurement campaign, and that the relaxation is governed by the exchange reaction. Neither assumption is guaranteed, and the checks below test them only partly.
Pitfall 1 — the sample changes during the campaign
At the temperatures where exchange is conveniently fast (often 150–200 °C), other processes can run in parallel. It helps to name them separately, because they push the data in different directions:
- Chemical degradation (chain scission, oxidation, hydrolysis) usually lowers the modulus and speeds up apparent relaxation.
- Post-curing (residual functional groups still reacting) usually raises the modulus and slows relaxation.
- Physical changes (loss of plasticiser, solvent or moisture; changes in crystallinity or phase structure) can move the modulus either way.
- Measurement artefacts (wall slip, loss of contact as the sample shrinks, normal-force drift, thermal expansion of the fixture) can mimic any of the above.
Screening check: before the relaxation series, run a time sweep (small-amplitude oscillation at constant temperature) at the highest planned temperature, for at least as long as the whole series will keep the sample hot. Choose a frequency well above the inverse relaxation time at that temperature, otherwise the sweep simply records the exchange-driven relaxation you intend to measure.
What it can and cannot tell you: a stable G′ is reassuring, but it does not prove that nothing happened. Opposing processes (for example scission and post-curing) can cancel in the modulus, and a small-strain measurement is insensitive to some changes that matter under the larger strains of a relaxation step. A drifting G′ shows that the sample is evolving; on its own it does not say which of the processes above is responsible.
Pitfall 2 — sequential temperature protocols
The common protocol steps through temperatures in order, high → low or low → high. Each measurement then inherits the cumulative thermal history of the ones before it, so if the sample evolves, temperature and time-at-temperature are confounded by design.
Screening check: use fresh samples where practical, or randomise the temperature order across at least two specimens (for example high–low–mid on one and mid–high–low on another). Returning to the first temperature at the end of the series is a simple additional test: the relaxation time measured there should reproduce the first value within the repeatability of the method.
Pitfall 3 — trusting a straight Arrhenius plot
A linear ln τ versus 1/T plot can still be misleading. A sample that changes steadily during a sequential protocol can produce a convincingly straight line with a shifted slope. Linearity is necessary, not sufficient.
Screening check: compare the activation energies obtained from the sequential and the randomised protocols.
- Agreement within uncertainty is reassuring evidence that the history of the sample did not dominate the result. It has limited diagnostic power: a process that changes the sample at the same rate in both protocols would go undetected.
- Disagreement shows that the result depends on the protocol. It is a reason to investigate, not an identification of the cause. Any of the processes in Pitfall 1 could be involved.
Controls that distinguish the causes
When the screening checks raise a doubt, compare specimens before and after a heating cycle identical to the measurement campaign:
- FTIR (or NMR on soluble fractions) for new or consumed functional groups: oxidation products, residual reactive groups, changes in the exchangeable bonds themselves.
- DSC for residual curing exotherms or shifts in Tg.
- TGA, or simply weighing the specimen, for loss of volatiles.
- Gel fraction and swelling ratio for net scission or additional crosslinking.
- Repeating the measurement under inert gas to test whether oxidation contributes.
A separate question: what the activation energy describes
Even in a perfectly stable sample, the apparent activation energy obtained from stress relaxation describes bulk flow of the network. It is not automatically the activation energy of the exchange reaction measured on small-molecule model compounds. El-Zaatari, Ishibashi and Kalow showed that changing the cross-linker in a vitrimer altered relaxation times by orders of magnitude while leaving the flow activation energy essentially unchanged: the differences appeared in the pre-exponential factor rather than in the slope (see References). Network architecture, the exchange mechanism (associative or dissociative) and mobility of the reacting groups can all contribute. Report the value as an apparent (flow) activation energy and compare it with model-compound kinetics explicitly rather than assuming they coincide.
The habit worth keeping
Report the time sweep, the protocol order and any before/after characterisation alongside the relaxation data. They cost a few experiments and make it possible for a reader to judge what the activation energy actually describes.
References
- D. Montarnal, M. Capelot, F. Tournilhac and L. Leibler, “Silica-like malleable materials from permanent organic networks”, Science 2011, 334, 965. doi:10.1126/science.1212648
- B. M. El-Zaatari, J. S. A. Ishibashi and J. A. Kalow, “Cross-linker control of vitrimer flow”, Polym. Chem. 2020, 11, 5339. doi:10.1039/D0PY00233J